Research/Sitter/MAGNDATA / 0.188_CeMnAsO.mcif

⬇ Download .mcif  ·  Data (JSON)

Spin lattice of CeMnAsOSpin lattice of CeMnAsO

CeMnAsO

MAGNDATA entry 0.188 · source
noncollinear antiferromagnet
All moments add up to a net magnetisation: an ordinary magnet. Spin splitting is the same in every direction (s-wave).
ordered ≤ 7 K (−266 °C)Colour: where that sits relative to 25 °C. Saturation: how much margin it has.
Structure · 10 properties
Magnetic groupP2′/c BNS 13.67
Parent space groupP 4/n m m No. 129
Spinscoplanar · net moment 0 μB per cell
Propagation[0 0 0] 1k
Cella 4.0837 · b 4.0837 · c 8.9567 Å · α 90° · β 90° · γ 90°
Transition7 K (−266 °C)
Measured at2 K
Magnetic ionsCe, Mn
Largest moment component3.32 μB
MethodNPD

Symmetry

Stereogram of the magnetic point group: each operation applied to one direction. Filled = upper hemisphere, ring = lower; red operations include time reversal. Lines are mirrors; polygons are 2/3/4/6-fold axes; the centre ring is inversion.

Every structure in P2′/c →
Atom sites · 4 sites · CSV
siteelementxyzmambmc|m| (μB)
Ce1Ce0.250.250.12870.70.300.7616
Mn1Mn0.750.250.5−3.32003.32
As1As0.250.250.672
O1O0.750.250

Moment components are along the crystal axes a, b, c (μB), as magCIF writes them. Symmetry generates the rest of the cell from these sites.

Source

Q. Zhang et al. PHYSICAL REVIEW B (2015) · doi:10.1103/PhysRevB.91.064418

Cite the original paper and MAGNDATA, not this mirror.

Original file

⬇ 0.188_CeMnAsO.mcif from MAGNDATA · entry page

sha256 of this copy: 133f360efaf41df8ca63426955fe04dac0374a7e6dc0337e762e46a8136a3ecc
The mirror keeps the bytes Bilbao served, so the original should hash the same unless MAGNDATA has revised the entry since: shasum -a 256 0.188_CeMnAsO.mcif.